Sunday, 9 August 2009

Triax CaO_MgO_Li2O Cobalt Green glaze


Triaxial analysis of FLUX Triax CaO_MgO_Li2O Cobalt Green glaze.
Fired to Cone 10 in Oxidation on LF18 white firing Clay

KNO_CaO Fritt Line Blend



This line blend is exchanging KNO for CaO with Tile A with the most Calcium present and Tile B with the most KNO present.
B2O3 is present as is Alumina and Silica at constant levels. This set of tests have yielded some well melted and slightly fluid results.The colour has a definite pattern of being very strong greeny blue at Tile A and changing to an apple green at Tile B where the KNO becomes more dominant.Generally the tiles have remained shiny due to the Boric oxide adding glass to the matrix, and lowering the maturing temp.It may also have an influence
on colour in the background as it acts as a solvent and disperses colour

KNO_LiO2





This Flux combination of Li2O and CaO has interesting colour changes Shiny durable surface..where Calcium is present and as it decreases and the Lithium increases the surface becomes less shiny and the colour becomes a mossy green.and a dull surface.The surface becomes less durable as it increases with the lithium until it finally shivers off the test at tiles 2-A
Tile 6 stands out as being very different and has a beautiful depth of colour and a non crazed durable surface.I would like to test this combination further for my Cobalt green Glaze project.it seems that tile B and six are very different colourwise. Tile B Has Calcium only and turned blue and does not have any lithium in it. Tile 6 has Calcium and some Lithium and it seems that Lithium helps turn cobalt green .of course it still maybe a thickness of application. but it does have exciting connotations.

KNO__ZnO



This flux combination has KNO decreasing and ZnO increasing from A-B.
Generally this combination has produced shiny viscous glazes moving towards a matt opaque surface which has cracked and likely to peel off caused by the excess of Zinc Oxide which has a a low COE..It has also suppressed the Cobalt Carbonate allowing the Rutile to be more active.creating a more yellowish colour moving to a pale green as it has become matt. In the earlier samples the glaze has a very strong durable shiny quality Tile 5 is still shiny but has started to crawl

KNO_SrO Line Blend



This line blend consists of removing Potassium and adding Strontium.This Combination of Flux created a very inconsistent pattern of texture with very rough ,bubbly unpleasant and shiny to smooth and onto dull and matt. Where the surface quality of the tests were smooth the colour was a bright blue, tiles T3-T6 the Tiles A-2 were coarse and variegated showing some bright green Tile &B was a dull matt with a greenish hue. As a dominant flux produces eventually a matt surface. These fluxes combined are both strong fluxes and their combined fluxing power may have caused the rough bubbly surface and as the power of the flux was decreased with the KNO reduction the glaze smoothed out to eventually become matt and colour suppressed.

Line Blend of KNO_MgO




This Line blend consists of Magnesium replacing Potassium and Sodium.Generally the Colour was muted and the surface moved from shiny opaque to very matt and opaque the colour decreased as the magnesium increased There was no Crazing present and the glaze had a thick glutanous and viscous surface. Magnesium has a low fluxing power and as the amount of MgO increased towards tile 7 the glaze melted less and had less tensile strength and started to flake off tiles 6 and 7,Could also be to do with less shrinkage as well as it has a low coefficient of expansion

In search of Shiny Cobalt Titanium Greens

Line blend shows Calcium Oxide replacing Potassium and Sodium (KNO)


with Alumina and Silica remaining constant...
Cobalt Carb 2% and Rutile 6% is added to all tests.Fired to Cone 10 Oxidation.