Tuesday, 11 August 2009

You got to be dedicated to do this stuff









































Me in my glaze room,I am currently working on another triaxial for Shiny Cobalt greens..I am making a triaxial of Tile 2 ( FLUXT CAO_MGO_LIO__#2)and trying to identify whether it is the Ratio of the Colourants that change Cobalt from Blue to green or Titanium changing it from yellow to Green and OR whether it is the glaze base and interchangeable fluxes as shown in previous triaxials.
Here are the 3 corners of the triaxial

The Ceramic Chicken was made by layering thin pieces of textured clay, I made moulds of unusual textures using Latex.
High fired stoneware in a gas kiln


High fired stoneware..I wrap large pieces of slabbed clay around cardboard tubes and place on slab of clay and remove cardboard,it helps to have sheets of newspaper on the tube to ease removal and when firm enough remove tube and shape with a damp piece of chamois leather.

Sunday, 9 August 2009




Generally with this colour combination of Cobalt/Rutile calcium needs to be present to obtain some Blue otherwise it changes to green or grey with magnesium and lithium present


From Corner C to B is a line blend of Lithium (C) and Magnesium (B)
This line blend contains no Calcium and has the colour has muted pale Blue at Corner B(T16) The colour in this line blend progressive from very opaque Blue grey to some beautiful shinier greys @ tiles17,18 and 19.and onto a shiny green as it interacts as the Lithium increases and the surface deteriorates at Tiles 20 and 21.Lithium seems to be a valuable secondary flux in smaller proportions adding melt and unusual colour but is not so useful in larger amounts.

From Corner A to Corner C is a line blend of Calcium (A) and Lithium (C)
Again Cnr A(Tile 1) is a Shiny Dark blue green and well melted which quickly changes to a lighter blue green variegated glaze when small amounts of lithium are introduced at T3.The tiles still remain shiny and well melted through to Tile 21.Changes to colour and texture are quite obvious along this line blend and Blue changes to apple green at T6 pinholing starts at T6 and progressively starts to melt and move.Lithium is known to produce bubbles in the glaze melt .At Corner C(Tile21) the glaze has shivered due to the small molecule size of Lithium that causes it to be mobile and it migrates to the Alumina and silica of the body and creates an interface of low expansion glass which peels off.Tile 3 is very beautiful and worth pursuing and developing.The others in the Lithium Line blend have lovely colour but the texture and surface are mostly marred by pinholing or shivering

More on Search for shiny Cobalt greens

General Observations of this triaxial Glaze are.
The glaze is a mostly stable and shiny glaze except at 2 corner Tiles A and C where the fluxes of Calcium and Lithium are predominant and Lithium has become fluid. Corner B is Matt. magnesium. The Blue green colour changing from Dark blue at Corner A to Pale blue at Corner B and Aqua green at C.




From Corner A to Corner B is a line blend of Calcium and Magnesium.
At Cnr A where Calcium is predominant the Glaze is very shiny well melted and Dark blue green it has started to move on the back of the tile this line blend progresses towards Cnr B with Magnesium becoming predominant and the surface has become more muted and becomes opaque.caused by the excessive magnesium.This line has no Lithium in its make up but has remained shiny except T16 and has no crazing.Tiles 1-11 are very interesting glaze tests.
My Colourants were Cobalt Carbonate 2.% and Rutile 6%.